In Materials Science and Engineering we often speak of
elastic stress effects.
By elastic stress we mean the stress that
arises from the elastic part of the strain,
\(\sigma_{ij}=C_{ijkl}(\epsilon_{kl}-\epsilon^0_{kl})\), where
\(\epsilon^0\) is the eigenstrain from coherent misfit. We use this
idea to understand the microstructural patterns that form in elastically
coherent solids. A hard-core mechanician will politely remind us that stress is
stress: it does not come in elastic and plastic flavours. Fair enough. We
accept the correction, and then carry on saying “elastic stress effects”
anyway, as materials scientists have for decades. For us, “elastic stress”
is shorthand for where the stress comes from, not a new kind of stress.
In this laboratory, you can explore these effects yourself: change the misfit strains, elastic constants and particle shape to calculate stresses and elastic energies. We explain the equations and compare the results with examples from my thesis and our research papers. Every calculation follows my teaching and research formulations, and you can check the validation tests and source code yourself.
Built with contributions from my former PhD students Tushar Jogi, Sandeep Sugathan and Soumya Bandyopadhyay; read about their work.
Coherent spinodal decomposition with elastic anisotropy (\(A_Z=3\), 1% misfit, 256 × 256). Elastic stress aligns the domains along the elastically soft x and y directions. You can run this simulation yourself.
Modules I–V use two-dimensional small-strain elasticity; Module 0 uses the
full three-dimensional stiffness. Crystal axes: x = [10], y = [01].
Shape and eigenstrain are prescribed; these experiments calculate energies
and orientations, not a complete evolving microstructure. All numerical
inputs use consistent dimensionless units.
Each module has its own inputs. Changing or resetting one module does not
change another. Try these values recalculates that module; Reset this module
restores its initial values.
MODULE 0
Elastic constants and mechanical stability
When is a crystal mechanically stable?
Elastic constants relate elastic strain to stress:
\(\sigma_{ij}=C_{ijkl}e_{kl}\). Here \(\sigma_{ij}\) is stress in pascals,
\(e_{kl}\) is dimensionless elastic strain, and \(C_{ijkl}\) is stiffness
in pascals. The indices identify Cartesian components. The elastic energy
per volume is \(w=\tfrac12 C_{ijkl}e_{ij}e_{kl}\), in joules per cubic
metre. The numerical examples below use a common scaled energy-density
unit rather than a specified material.
Principal stresses and strains
We can describe the same strain or stress using different coordinate axes. The components change when we turn the axes, even though the material state stays the same. Some directions make the description especially simple: the shear components vanish. These are the principal directions.
A principal strain is the normal strain along one of these directions. A positive value means extension; a negative value means contraction. A principal stress is the normal stress on a plane whose normal follows a principal direction. On that plane, the traction has no tangential, or shear, component. Positive stress here means tension.
The examples below are two-dimensional. In three dimensions, a symmetric stress or small-strain tensor has three mutually perpendicular principal directions. If two principal values are equal, their individual directions within that plane are not unique.
Principal strains: the same deformation, different axes
We start with pure shear: \(e_{xx}=e_{yy}=0\) and \(e_{xy}=e_{yx}=-q\), with \(q=0.01\). The strain is small and dimensionless. Its engineering shear is \(\gamma_{xy}=2e_{xy}=-0.02\); the factor of two is a convention, not a different deformation.
The dashed square has edges along the original \(x,y\) axes. Pure shear makes it a rhombus. We magnify the shape change 12 times to make it visible. The blue rhombus stays fixed while we turn only the measuring axes.
An eigenvector identifies a direction that the strain tensor maps back onto the same line. Its eigenvalue is the normal strain along that direction. These are the principal strain directions and principal strains. We find them by turning the axes until the shear component vanishes.
Try the slider, then select Align axes with eigenvectors. Watch the off-diagonal entries shrink to zero. The new axes follow extension along one diagonal and contraction along the other.
In this example the eigenvectors are \(\mathbf n_1=(1,-1)/\sqrt2\) and \(\mathbf n_2=(1,1)/\sqrt2\). A unit vector has length one, so these vectors specify directions without adding a length scale. The strain tensor maps each one back onto its own line:
An eigenvector gives the direction; its eigenvalue gives the normal strain along it. Here the eigenvalues are \(+0.01\) and \(-0.01\): 1% extension and 1% contraction. A negative principal strain is physical; it means contraction.
Putting these eigenvectors along the new axes gives the diagonal matrix \(\operatorname{diag}(q,-q)\). This is the same physical strain as the off-diagonal matrix, expressed in its principal directions. At \(+45^\circ\), the entries are swapped; both choices are principal axes.
A square initially aligned with these principal axes would become a rectangle. The square drawn here was initially aligned with the original axes, so it becomes a rhombus. Rotating the measuring axes does not change that rhombus into a rectangle.
Why does the matrix change?
The columns of \(\mathbf Q\) are the new unit axes expressed in the original coordinates. For an angle \(\theta\),
The superscript \(T\) means transpose: exchange rows and columns. Multiplying by \(\mathbf Q\) and \(\mathbf Q^T\) expresses the same tensor in the new axes. When the columns of \(\mathbf Q\) are eigenvectors, the off-diagonal terms vanish.
Stress: turn the planes on which we resolve traction
We start with \(\sigma_{xx}=80\), \(\sigma_{yy}=20\), and \(\sigma_{xy}=\sigma_{yx}=30\), all in MPa. One MPa is one million pascals.
The square represents an imaginary cut element. Rotating it selects different planes within the same stress field; we are not rotating the material or changing the load.
At the principal directions, the orange shear arrows disappear. Only normal traction remains on these faces. Shear can still act on other planes; principal directions do not mean that shear is absent everywhere.
How do eigenvectors enter?
A unit vector is a direction vector of length one. If \(\mathbf n\) is a principal direction, applying the tensor gives a vector along that same line:
The direction \(\mathbf n\) is an eigenvector. Its multiplying factor, \(e_i\) or \(\sigma_i\), is an eigenvalue: the principal strain or principal stress. For stress, \(\boldsymbol\sigma\mathbf n\) is the traction on the plane with normal \(\mathbf n\). When it is parallel to the normal, it has no shear component.
We use separate illustrative stress and strain states here, rather than a paired constitutive calculation. In isotropic linear elasticity, stress and elastic strain share principal directions. In anisotropic elasticity they need not. Principal elastic strain directions also need not match those of the total strain if an eigenstrain is present.
Which elastic constants describe a stable crystal?
The principal strains above can be positive or negative: extension and contraction are both allowed. We now ask a different question. Does every small elastic distortion of an unstressed reference crystal cost energy? If it does, that reference state is elastically stable.
The stiffness matrix is positive definite when its quadratic elastic energy is positive for every nonzero elastic strain. Its eigenvalues describe the energy cost of strain modes. They are not the principal strains or principal stresses introduced above.
Write the energy as a sum of independent mode contributions
A symmetric strain tensor has six independent components in three dimensions. We collect them into an orthonormal component vector:
The factors \(\sqrt2\) account for the two equal off-diagonal tensor entries, such as \(e_{xy}=e_{yx}\). This convention is often called Kelvin notation. It preserves \(\mathbf s^T\mathbf s=\boldsymbol e:\boldsymbol e\). Here \(\mathbf K\) is the stiffness matrix in this convention, and \(T\) means transpose.
Because the stiffness comes from a quadratic elastic energy, \(\mathbf K\) is symmetric. It therefore has an orthonormal set of eigenvectors \(\mathbf v_\alpha\). Each eigenvector specifies a combination of strain components, or a strain mode. We can write any strain as a sum of these modes:
The coefficient \(a_\alpha\) is the amount of mode \(\alpha\) in the strain. Substituting this sum into the energy and using \(\mathbf v_\alpha^T\mathbf v_\beta=0\) for different modes, and 1 for the same mode, removes the cross terms:
Every squared amplitude is nonnegative. If all \(\lambda_\alpha>0\), every nonzero strain raises the energy. If one eigenvalue is negative, choosing just that mode gives negative energy relative to the unstrained state: the reference state is unstable. A zero eigenvalue gives no quadratic restoring energy for that mode and fails strict positive definiteness.
Thus the small-strain stability requirement is \(\mathbf K\) positive definite, or equivalently, all its eigenvalues strictly positive. These conditions apply to an unstressed reference state. Stability under finite applied stress requires additional care.
For a cubic crystal, only three combinations need checking
In the same orthonormal convention, the cubic stiffness matrix separates into a normal-strain block and three independent shear modes:
Multiplying the normal block by \((1,1,1)^T\) gives \((C_{11}+2C_{12})(1,1,1)^T\): equal normal strains form the volume-change mode. Multiplying it by \((2,-1,-1)^T\), or by \((0,1,-1)^T\), gives the same vector multiplied by \(C_{11}-C_{12}\). These are two independent normal-strain modes with zero trace. The three shear eigenvalues are \(2C_{44}\).
The full set is therefore \(C_{11}+2C_{12}\) once, \(C_{11}-C_{12}\) twice, and \(2C_{44}\) three times. Requiring them all to be positive gives exactly the three cubic inequalities below. The deformation curves then show what each inequality means physically.
In engineering-shear notation the shear diagonal entries are \(C_{44}\), because the strain coordinates use \(2e_{xy}\) instead of \(\sqrt2e_{xy}\). The numerical shear eigenvalues depend on that coordinate convention; the positive-definiteness conditions do not.
Why do other crystal symmetries have more complicated conditions?
The energy argument is the same for every symmetry. Cubic symmetry simplifies the eigenvalues into three combinations. With less symmetry, additional constants couple different normal or shear strains. Positive diagonal entries alone cannot guarantee positive energy for a coupled distortion.
For example, a two-mode energy contains \(a x^2+2bxy+c y^2\). Completing the square gives
\[a x^2+2bxy+c y^2=a\left(x+\frac ba y\right)^2+\left(c-\frac{b^2}{a}\right)y^2.\]
It is strictly positive for every nonzero pair when \(a>0\) and \(ac-b^2>0\). The coupling \(b\) cannot be arbitrarily large, even when both diagonal coefficients are positive.
For hexagonal and tetragonal-I crystals, take \(r=(e_{xx}+e_{yy})/\sqrt2\) and \(z=e_{zz}\). Their coupled normal block is
The same square-completion argument gives \((C_{11}+C_{12})C_{33}-2C_{13}^2>0\), alongside positivity of the other independent modes. This explains the quadratic condition in the symmetry table. For a general symmetric stiffness matrix, one can check all eigenvalues, or equivalently require all leading principal minors to be positive. A leading principal minor is the determinant of a top-left square block, taking successively one, two, and then all six rows and columns.
Cubic crystals: three independent stiffness constants
The first condition resists a tetragonal distortion that preserves volume to first order. The
second gives a positive bulk modulus \(K=(C_{11}+2C_{12})/3\), which
resists uniform compression. The third resists shear in the principal
planes. The normal-strain block has eigenvalues \(C_{11}+2C_{12}\) and
\(C_{11}-C_{12}\), the latter occurring twice. The three orthonormal shear-mode eigenvalues are \(2C_{44}\). Stiffness eigenvalues and \(K\) use the same units
as the stiffnesses.
The dimensionless Zener ratio measures cubic elastic anisotropy. The
equality gives an isotropic elastic tensor within the cubic law. A cubic
crystal is not automatically isotropic.
Convert between stiffnesses and Schmidt–Gross parameters
Following I. Schmidt and D. Gross, Sandeep’s thesis uses the average
in-plane shear modulus \(G\), the effective Poisson parameter \(\nu\), and
\(A_Z\). Here the same average shear parameter is labeled \(\mu=G\).
Specifically, \(\mu\) is the angular average of the rotated \(C_{1212}\)
in the (001) plane, and \(\nu=\Lambda/[2(\Lambda+\mu)]\), where
\(\Lambda\) is the angular average of the rotated \(C_{1122}\). These are
averaged parameters, not the shear modulus and Poisson ratio for every
direction in an anisotropic crystal.
At \(A_Z=1\), the mapping becomes the usual isotropic law: \(C_{44}=\mu\),
\(C_{12}=2\mu\nu/(1-2\nu)\), and \(C_{11}=2\mu(1-\nu)/(1-2\nu)\). For the
anisotropic mapping with \(\mu>0\), \(A_Z>0\), and \(\nu<1/2\), cubic
stability additionally requires \(1+3A_Z+4\nu>0\). We check the
converted stiffnesses against the stability conditions. Module IV uses a fixed \(\nu=1/3\);
the other conversion panels permit changing \(\nu\).
Change this calculator’s constants directly or use the equivalent
parameters. It does not change another module. Try an unstable case to see
which deformation loses its restoring energy.
What does strain amplitude mean?
We start with the same cubic crystal and apply three different distortions. Move the strain slider to compare the original cube on the left with the deformed crystal on the right. The matching colored dots on the energy curves show the energy at the selected strain.
The sketches magnify the shape changes 30 times so they are visible. The curves and energy values use the actual strain, not the magnified value. These are schematic crystal blocks, not atomistic simulations.
Horizontal axis: strain amplitude \(q\). Vertical axis: elastic energy per volume, relative to the unstrained crystal, in model energy-density units.
Curvature, an energy minimum and stable equilibrium
At \(q=0\), the crystal is unstrained. Each curve has zero slope there, so there is no first-order energy change: this is an equilibrium point. Its stability depends on what happens when we give the crystal a small strain in either direction.
An upward-opening curve has positive curvature. Moving away from zero toward either positive or negative \(q\) raises the energy. The bottom of the curve is therefore an energy minimum. The crystal resists a small distortion and tends to return toward the minimum: this is stable equilibrium with respect to that strain mode.
A downward-opening curve has negative curvature. A small positive or negative strain lowers the energy, so \(q=0\) is an energy maximum along that path. A small disturbance is favored rather than resisted: the equilibrium is unstable with respect to that mode.
For these quadratic curves, \(w(q)=a q^2\), where \(w\) is elastic energy per volume and \(a\) is the coefficient for the chosen strain path:
The second derivative gives the sign of the curvature. If \(a>0\), the energy has a minimum. The restoring tendency is proportional to \(-dw/dq=-2aq\), which points back toward zero. If \(a<0\), that tendency points away from zero. A flat curve has \(a=0\): there is no quadratic restoring energy. It marks the boundary of strict elastic stability; higher-order terms would be needed to decide behavior beyond this quadratic model.
Stable cubic elasticity requires all three energy coefficients to be positive. One negative mode is enough for instability, even if the other curves bend upward. The unstable-stiffness button above gives an example. A steeper curve means more energy along that particular strain path; the same \(q\) does not give the same total strain magnitude in all three examples.
The graph uses strain amplitude \(q\), which is dimensionless. Uniform
dilation has \(e_{xx}=e_{yy}=e_{zz}=q\); tetragonal distortion has
\(e_{xx}=q,e_{yy}=e_{zz}=-q/2\); simple shear has engineering shear
\(\gamma_{xy}=q\), so tensor shear is \(e_{xy}=q/2\). All other components
vanish in each example. In the tetragonal example, the two transverse edges remain equal. The strain trace is zero, so volume is unchanged to first order. The plotted energies are respectively
\(\tfrac32(C_{11}+2C_{12})q^2\), \(\tfrac34(C_{11}-C_{12})q^2\), and
\(\tfrac12C_{44}q^2\).
Other crystal symmetries
The following are three-dimensional stiffness conditions. The later
widgets use the in-plane cubic sub-block; they are not hexagonal or
tetragonal solvers.
Crystal symmetry
Independent constants
Stability conditions
Hexagonal
5
\(C_{11}>|C_{12}|\), \(C_{44}>0\), and
\((C_{11}+C_{12})C_{33}>2C_{13}^2\). Here
\(C_{66}=(C_{11}-C_{12})/2>0\) follows from the first condition.
Tetragonal I (4/mmm)
6
\(C_{11}>|C_{12}|\), \((C_{11}+C_{12})C_{33}>2C_{13}^2\),
\(C_{44}>0\), \(C_{66}>0\). Here \(C_{66}\) is independent.
Lower-symmetry tetragonal classes require an additional condition
involving \(C_{16}\).
Orthorhombic
9
\(C_{44},C_{55},C_{66}>0\); for the normal block, \(C_{11}>0\),
\(C_{11}C_{22}-C_{12}^2>0\), and
\(\det\begin{pmatrix}C_{11}&C_{12}&C_{13}\\C_{12}&C_{22}&C_{23}\\C_{13}&C_{23}&C_{33}\end{pmatrix}>0\).
Positive diagonal entries alone are insufficient.
A crystal is mechanically stable only if every small strain costs elastic energy. For cubic symmetry this reduces to three checks: \(C_{44}>0\), \(C_{11}-C_{12}>0\) and \(C_{11}+2C_{12}>0\).
MODULE I
Misfit and the habit line.
Along which line can a misfitting plate fit the matrix without strain?
Eigenstrain is the deformation a phase would adopt if unconstrained.
Elastic strain is the part left after subtracting that eigenstrain from
the compatible total strain.
Construct Mohr’s circle of strain.
Axes below are strain divided by \(\epsilon_\eta\). The vertical
coordinate is tensor shear \(\epsilon^0_{nq}\), not engineering shear
\(\gamma^0_{nq}=2\epsilon^0_{nq}\). While θ follows the zero-extension
line, P stays on a green intersection as t changes. Type a measurement
angle above to release it and move the point around the circle.
Why did this happen?
Physics: eigenstrain, Eshelby’s inclusion and the habit line
Eigenstrain
Eigenstrain is the stress-free transformation strain \(\epsilon^0\).
When a region transforms with no external constraint, its stress stays
zero:
\[\sigma=C:(\epsilon-\epsilon^0)=0,\]
where \(C\) is the elastic stiffness tensor and \(\epsilon\) the total
strain. In the free region the total strain equals the transformation
strain, \(\epsilon=\epsilon^0\). Examples are the lattice-misfit
dilatation of a precipitate,
\(\epsilon^0_{ij}=\delta_{ij}(a_p-a_m)/a_m\), thermal expansion, and the
spontaneous distortion of a lattice during a phase change. In this
module \(\epsilon^0=\epsilon_\eta\,\mathrm{diag}(1,t)\) in the crystal
axes: principal strains \(\epsilon_1=\epsilon_\eta\) along [10] and
\(\epsilon_2=t\,\epsilon_\eta\) along [01].
Eshelby’s four steps
To find the stress when the transforming region is constrained by a
surrounding elastic matrix, Eshelby (1957) used a thought experiment:
Cut the region Ω (the inclusion) out of the matrix
and let it undergo its stress-free transformation \(\epsilon^0\).
Apply surface tractions to force it back into its
original hole. This imposes elastic strain \(-\epsilon^0\), i.e.
stress \(-C:\epsilon^0\).
Weld the interface back together.
Release the tractions. The inclusion and the matrix
relax together to mechanical equilibrium.
The relaxation leaves a constrained total strain \(\epsilon^c\) inside
the inclusion. The elastic strain is the difference between the
constrained and the stress-free geometry, and only it stores energy:
\[e=\epsilon^c-\epsilon^0,\qquad \sigma=C:e,\qquad w=\tfrac12\,e:C:e\ \
\text{(energy per unit volume)} .\]
For an ellipsoidal inclusion (an ellipse in 2-D) in a homogeneous
infinite matrix, Eshelby proved that \(\epsilon^c\) is uniform and
linear in the eigenstrain, \(\epsilon^c=S:\epsilon^0\). The Eshelby
tensor S depends on the inclusion’s shape and orientation and on the
elastic constants. This is where orientation dependence comes from: the
same \(\epsilon^0\) costs different energy in differently oriented
inclusions.
Figure 1. Eshelby’s thought experiment for an
inclusion with \(t<0\): it wants to stretch along x and shrink
along y. After step 4 the inclusion sits between its free shape and
its hole.
Thin-plate limit: a negotiation at the interface
Eshelby’s theory is a negotiation of space. The transformed region wants
a new shape; the surrounding matrix resists. The theory decides who
yields, and where stress is left trapped. For a very thin plate (a
martensite lath, a plate-shaped precipitate) the whole negotiation
happens at the flat interface. The plate is long compared with its
thickness, so the matrix, which extends far beyond the plate and is
unstrained away from its ends, dictates what happens along the plate.
Across its thickness, the plate is free to relax.
Why jump conditions appear at an inclusion
The eigenstrain switches on abruptly at the interface: it is zero in the
matrix and \(\epsilon^0\) in the plate. Suppose every strain and stress
component were continuous across the interface. Hooke’s law,
\(\epsilon^0=\epsilon-C^{-1}:\sigma\), would then make the eigenstrain
continuous as well. It is not. So some components of strain or stress
must jump. Two physical laws decide which ones:
No tearing, no overlapping. The interface is welded,
so the displacement is continuous. This constrains the strain.
Newton’s third law. The force that the plate exerts
on the matrix across the interface equals and opposes the force the
matrix exerts on the plate. This constrains the stress.
The interface handshake
1. The matrix rules the length (Hadamard kinematics).
Plate and matrix cannot separate, so their displacements match
everywhere along the interface direction \(\mathbf s\). Their
derivatives along \(\mathbf s\) then match too, and the plate’s total
strain along the interface equals the matrix value: \(\epsilon_{ss}=0\).
The plate is still free to thicken, thin or shear across its thickness
(direction \(\mathbf m\)). That freedom is a jump in the displacement
gradient of the form \(\mathbf b\otimes\mathbf m\), where \(\mathbf b\)
is not yet known.
2. The forces rule the thickness (traction continuity).
The forces pushing, pulling and sliding across the interface must
balance. So the traction vector \(\sigma\mathbf m\), which contains the
normal stress \(\sigma_{mm}\) and the shear stress \(\sigma_{sm}\), is
continuous. No balance law acts on the stress that stretches the plate
along its length, \(\sigma_{ss}\): it may differ completely from the
matrix value.
Across the welded interface, each component is fixed by exactly one law.
When the strain component is fixed, the matching stress component may
jump, and the other way round:
component
strain \(\epsilon\)
stress \(\sigma\)
ss (along the plate)
continuous: Hadamard (matches the matrix)
free to jump: remnant stress
sm (shear)
free to jump: set by \(\mathbf b\)
continuous: traction
mm (across the plate)
free to jump: set by \(\mathbf b\)
continuous: traction
Counting. In 2-D a symmetric strain has 3 components.
Hadamard fixes 1 of them (\(\epsilon_{ss}\)); the other 2 are carried by
the 2 unknown components of \(\mathbf b\). Traction continuity supplies
2 equations (\(\sigma_{sm},\sigma_{mm}\)), exactly enough to find
\(\mathbf b\). In 3-D: 6 strain components, 3 fixed in-plane by
Hadamard, 3 carried by \(\mathbf b\), and 3 traction equations to find
them.
Figure 2. The interface handshake. (A) A material
element of the plate may shear and thicken, \(\nabla\mathbf u=\mathbf
b\otimes\mathbf m\), but keeps its length along \(\mathbf s\). (B) A
thin pillbox straddling the interface: the traction on its two faces
must balance, while the stress along \(\mathbf s\) may differ on the
two sides. (C) After relaxation the faces are traction-free, and only
\(\sigma_{ss}\) remains.
Duality and the remnant stress
The unknown deformation \(\mathbf b\) and the interface traction
\(\sigma\mathbf m\) are work conjugates: a movement and the force that
resists it. Changing \(\mathbf b\) by \(\delta\mathbf b\) changes the
plate’s energy density by \(\delta w=(\sigma\mathbf m)\cdot\delta\mathbf
b\). So when the plate chooses \(\mathbf b\) to minimize its energy, the
traction on its faces is driven to zero: \(\sigma_{mm}=\sigma_{sm}=0\).
The plate relaxes completely across its thickness.
What is left is the stress along the plate. The plate is still held to
zero length change along \(\mathbf s\), although it wanted to change by
\(\epsilon^0_{ss}\). It carries the elastic strain
\(e_{ss}=-\epsilon^0_{ss}\) and, because its faces are free, a single
uniaxial stress
where \(E_s\) is the (plane-strain) stiffness of the crystal along
\(\mathbf s\). This is the whole elastic penalty of a thin plate: the
remnant stress it pays for staying compatible with the matrix. It
vanishes only when \(\epsilon^0_{ss}=0\), on the habit line. In the
worked case of Step 7(vii) the plate wanted to shrink by 0.005 along
\(\mathbf s\), was held at its original length, and carries a tension of
0.0133. Figure 3 shows every component across that interface.
Figure 3. Profiles across the interface for the
worked case (Step 7(vii): isotropic C, plate along [01]). The
eigenstrain jumps in both components. Kinematics keeps the total
strain along the interface continuous; statics keeps the traction
continuous. The remaining components jump: the strain across the plate
(through \(\mathbf b\)) and the stress along it (the remnant stress).
Names
\(\mathbf n,\ \mathbf q\): an arbitrary pair of orthogonal unit
vectors defining a rotated frame; \(\mathbf n\) is at angle θ from
[10].
\(\mathbf s\): the invariant (habit) line direction, the value of
\(\mathbf n\) where \(\epsilon^0_{nn}=0\). Green line on the plot.
\(\mathbf m\): the habit normal, orthogonal to \(\mathbf s\); the
value of \(\mathbf q\) at that θ. Orange arrow on the plot.
“Habit angle” is used in the literature for both the line and the
normal, which differ by 90°. This page always says which.
Limits
The ideal plate theory assumes an infinitely long plate, a sharp
interface, a uniform transformation strain, linear small-strain
elasticity and a homogeneous stiffness. Real plates have ends, finite
thickness, interfacial energy and diffuse interfaces, and plasticity can
destroy coherency. In this laboratory, Module II replaces the ideal
plate by a finite elliptical inclusion with Eshelby’s full solution,
Module III adds elastic anisotropy, Module IV two phases with different
eigenstrains, and Module V plates stiffer or softer than the matrix.
Planned extensions. Future modules will relax the
remaining assumptions: inclusions stiffer or softer than the matrix
through Eshelby’s equivalent-inclusion method, interfacial energy and
phase-field gradients for diffuse interfaces and evolving shapes,
dislocation arrays for the loss of coherency, and the 3-D
invariant-plane analysis of the phenomenological theory of martensite
crystallography.
Mathematics: derivation, step by step
Small strain; crystal axes x = [10], y = [01]; repeated indices summed.
Vectors are columns.
Step 1. Rotate \(\epsilon^0\) into the \((\mathbf n,\mathbf q)\) frame.
In its principal frame the eigenstrain is diagonal,
\(\epsilon^0=\begin{pmatrix}\epsilon_1&0\\0&\epsilon_2\end{pmatrix}\). A
frame at angle θ has basis vectors and rotation matrix (rows = new basis
vectors)
Each new component is the tensor sandwiched between two basis vectors,
e.g. \(\epsilon^0_{nq}=\mathbf n^{\mathsf T}\epsilon^0\,\mathbf
q=n_i\,\epsilon^0_{ij}\,q_j\). All four at once are
\(\epsilon'=R\,\epsilon^0R^{\mathsf T}\). Multiply in full:
Check: the trace
\(\epsilon^0_{nn}+\epsilon^0_{qq}=\epsilon_1+\epsilon_2\) and the
determinant
\(\epsilon^0_{nn}\epsilon^0_{qq}-(\epsilon^0_{nq})^2=\epsilon_1\epsilon_2\)
do not change with θ. For this module put \(\epsilon_1=\epsilon_\eta\),
\(\epsilon_2=t\,\epsilon_\eta\):
\(\epsilon^0_{nn}=\epsilon_\eta(\cos^2\theta+t\sin^2\theta)\), the curve
in the “Normal eigenstrain along n(θ)” plot. At a habit root, \(\mathbf
n\) becomes \(\mathbf s\) and \(\mathbf q\) becomes \(\mathbf m\).
Step 2. Eshelby’s thin plate.
(a) Hadamard compatibility. Let the interface be the
plane with normal \(\mathbf m\). The displacement \(\mathbf u\) is
continuous across it, so its derivative along any direction \(\mathbf
s\) lying in the interface (\(\mathbf s\cdot\mathbf m=0\)) is the same
on both sides. The jump in the gradient therefore kills every in-plane
vector:
\[[\![\nabla\mathbf u]\!]\,\mathbf s=\mathbf 0\quad\text{for all
}\mathbf s\perp\mathbf m \qquad\Longrightarrow\qquad [\![\nabla\mathbf
u]\!]=\mathbf b\otimes\mathbf m,\qquad \mathbf b=[\![\nabla\mathbf
u]\!]\,\mathbf m .\]
The matrix far from the plate ends is unstrained, so inside the plate
\(\nabla\mathbf u=\mathbf b\otimes\mathbf m\). Here \(\mathbf b\) is an
unknown vector (a displacement per unit distance across the plate). In
index notation,
\[\frac{\partial u_i}{\partial x_j}=b_i\,m_j ,\]
where i labels the displacement component and j the direction of the
derivative. In 3-D, with \(\mathbf u=(u_1,u_2,u_3)^{\mathsf T}\),
\(\mathbf b=(b_1,b_2,b_3)^{\mathsf T}\) and \(\mathbf
m=(m_1,m_2,m_3)^{\mathsf T}\), the outer product is the column \(\mathbf
b\) times the row \(\mathbf m^{\mathsf T}\):
Every entry of the gradient is fixed by one component of \(\mathbf b\)
and one of \(\mathbf m\); for example the shear gradient \(\partial
u_1/\partial x_2=b_1m_2\). The matrix has rank one: every row is a
multiple of \(\mathbf m^{\mathsf T}\), so \(\nabla\mathbf u\,\mathbf
s=\mathbf b\,(\mathbf m\cdot\mathbf s)=\mathbf 0\) for any in-plane
\(\mathbf s\). Nothing changes along the interface. In this 2-D
laboratory \(m_3=b_3=0\) and the upper-left block remains:
\[\nabla\mathbf
u=\begin{pmatrix}b_1m_1&b_1m_2\\b_2m_1&b_2m_2\end{pmatrix},\qquad
\epsilon^c=\operatorname{sym}(\mathbf b\otimes\mathbf
m)=\tfrac12(\mathbf b\otimes\mathbf m+\mathbf m\otimes\mathbf b)
=\begin{pmatrix}b_1m_1&\tfrac12(b_1m_2+b_2m_1)\\\tfrac12(b_1m_2+b_2m_1)&b_2m_2\end{pmatrix}.\]
(b) Energy. The elastic strain is
\(e=\operatorname{sym}(\mathbf b\otimes\mathbf m)-\epsilon^0\). With
\(\sigma^0=C:\epsilon^0\) and the acoustic tensor \(Q_{ik}(\mathbf
m)=C_{ijkl}m_jm_l\), and using the symmetries of C,
The first term is the cost of forcing the plate fully back (Eshelby’s
step 2). The second is what it recovers by relaxing across its thickness
(step 4). Their difference is the elastic energy kernel \(B(\mathbf m)\)
of Module III and of Appendix A. In Eshelby’s language this is the
thin-plate limit, with \(S:\epsilon^0=\operatorname{sym}(\mathbf
b\otimes\mathbf m)\).
(d) The two jump conditions, derived. Let
\([\![f]\!]=f^{\rm plate}-f^{\rm matrix}\) denote a jump across the
interface. Kinematic: \(\mathbf u\) is continuous, so for any
in-plane \(\mathbf s\) the directional derivative is continuous,
\([\![\nabla\mathbf u]\!]\mathbf s=\mathbf 0\), which gives
\([\![\nabla\mathbf u]\!]=\mathbf b\otimes\mathbf m\) as in (a).
Static: apply \(\int_{\partial P}\sigma\,\mathbf n\,dA=\mathbf
0\) to a pillbox P of face area A straddling the interface. As its
height goes to zero the side faces vanish and only the two flat faces
remain:
With a homogeneous C, \([\![\sigma]\!]=C:\big(\operatorname{sym}(\mathbf
b\otimes\mathbf m)-[\![\epsilon^0]\!]\big)\), so the static condition
reads \(Q(\mathbf m)\,\mathbf b=(C:[\![\epsilon^0]\!])\,\mathbf m\).
These hold at every point of every coherent interface. For the thin
plate the matrix side is unstrained and
\([\![\epsilon^0]\!]=\epsilon^0\), which returns \(Q(\mathbf m)\mathbf
b=\sigma^0\mathbf m\) of (c): the thin-plate solution is the
pair of jump conditions.
(e) Duality. Vary \(\mathbf b\): \(\delta
w=\sigma:\delta e=\sigma:\operatorname{sym}(\delta\mathbf
b\otimes\mathbf m) =\delta b_i\,\sigma_{ij}m_j=(\sigma\mathbf
m)\cdot\delta\mathbf b\). The traction is the work conjugate of
\(\mathbf b\), so \(\partial w/\partial\mathbf b=\mathbf 0\) and
\(\sigma\mathbf m=\mathbf 0\) are the same statement.
(f) The remnant stress and a one-line energy. With
\(\sigma\mathbf m=\mathbf 0\), the only stress left in the \((\mathbf
s,\mathbf m)\) frame is \(\sigma_{ss}\): \(\sigma=\sigma_{ss}\,\mathbf
s\otimes\mathbf s\). Hadamard fixes \(\epsilon_{ss}=0\), so
\(e_{ss}=-\epsilon^0_{ss}\). Using the compliance \(S=C^{-1}\) (plane
strain), \(e_{ss}=S_{ssss}\,\sigma_{ss}\), hence
This is exact for any homogeneous stiffness, isotropic or anisotropic,
and it makes Step 3 immediate. For the isotropic law of this page
\(E_s=(C_{11}^2-C_{12}^2)/C_{11}=8/3\) in every direction, so
\(B=\tfrac83(0.005)^2=6.67\times10^{-5}\) for a plate along [01] and
\(\tfrac83(0.01)^2=2.67\times10^{-4}\) along [10], matching Step 7 and
the Module III curve. In an anisotropic crystal \(E_s\) depends on the
direction, which is how elastic anisotropy enters in Module III.
(g) Any coherent interface: the complete set of jump
conditions.
Steps (a)–(f) used a thin plate, but nothing in the jump conditions
depends on the plate. They hold at every point of any perfectly bonded
interface between an inclusion with uniform eigenstrain
\(\epsilon^0_{ij}\) (often written \(\epsilon^*_{ij}\)) and a matrix
with the same stiffness \(C_{ijkl}\). Let \(n_i\) be the outward unit
normal of the inclusion and \([\![A]\!]=A^{\rm in}-A^{\rm out}\), the
convention used on this page.
1. Displacement gradient. \(u_i\) is continuous, so only the
derivative across the interface can jump (Hadamard):
\[[\![u_{i,j}]\!]=g_i\,n_j .\]
2. Strain. The total strain is the symmetric part of the
gradient, and the eigenstrain jumps by its full value:
So the jumps are fixed locally by the normal, the stiffness and the
eigenstrain alone, whatever the shape of the inclusion. The shape only
decides the field on one side (Module II computes it for an ellipse).
Texts that define the jump as outside minus inside write
\(\lambda_i=-g_i\), and every jump below changes sign.
These are Hill’s discontinuity relations for a coherent interface (R.
Hill, “Discontinuity relations in mechanics of solids”,
Progress in Solid Mechanics 2, 247–276, 1961; see also Mura,
1987). For the thin plate, the matrix side is unstrained, so the plate’s
own field equals the jump and \(\mathbf b=\mathbf g\).
Step 3. \(B(\mathbf m)=0\iff\epsilon^0_{ss}=0\).
(⇒) If \(B(\mathbf m)=0\) then \(w=0\), and because C
is positive definite, \(e=0\): the total strain equals the
transformation strain, \(\operatorname{sym}(\mathbf b\otimes\mathbf
m)=\epsilon^0\). Project along the interface direction \(\mathbf s\)
(\(\mathbf s\cdot\mathbf m=0\)):
They match with \(a_s=2\epsilon^0_{sm}\), \(a_m=\epsilon^0_{mm}\). Then
\(\mathbf b=\mathbf a\) gives \(e=0\) and \(B(\mathbf m)=0\). The
condition is kinematic: it holds for every stiffness C. The elastic
constants only decide how costly the other orientations are.
Step 4. Solve for θ and the plate kinematics.
With \(\epsilon_1=\epsilon_\eta\), \(\epsilon_2=t\,\epsilon_\eta\) and
\(\cos\theta\ne0\):
A real root requires \(t\le0\) (\(t=0\) is the limit θ = 90°). On the
root \(\cos^2\theta=-t/(1-t)\), \(\sin^2\theta=1/(1-t)\) and
\(\sin\theta\cos\theta=\pm\sqrt{-t}/(1-t)\). Substituting into Step 1:
The upper sign is for \(\theta_1\), the lower for \(\theta_2\). The
rotation is the antisymmetric part of \(\mathbf a\otimes\mathbf m\):
\(\mathbf a\otimes\mathbf m=\epsilon^0+\epsilon^0_{sm}(\mathbf
s\otimes\mathbf m-\mathbf m\otimes\mathbf s)\). In units of
\(\epsilon_\eta\):
\(t=\epsilon_2/\epsilon_1\)
line θ₁ (θ₂)
thickening \(\epsilon^0_{mm}\)
shear \(2\epsilon^0_{sm}\)
rotation ω
ω for \(\epsilon_\eta=0.01\)
−1
45° (135°)
0
∓2.00
∓1.00
0.57°
−0.5
54.74° (125.26°)
0.50
∓1.41
∓0.71
0.41°
−0.25
63.43° (116.57°)
0.75
∓1.00
∓0.50
0.29°
0
90°
1.00
0
0
0
Step 5. Where \(\alpha=\tan^{-1}\sqrt{-t}\) comes from.
The habit condition can be written for the line or for the
normal. Both routes give the same plate.
Route A: start from the line. Step 4 gave the line
angle through \(\tan\theta_1=1/\sqrt{-t}\). The normal is the line
turned by 90°:
Route B: start from the normal. Call the normal angle
α, so \(\mathbf m=(\cos\alpha,\sin\alpha)\). The tangent is \(\mathbf
s=(-\sin\alpha,\cos\alpha)\). Put \(\mathbf s\) into the stretch formula
of Step 1 (the same sandwich \(\mathbf s\cdot\epsilon^0\mathbf s\)):
Route B is the form you meet when the energy is written in terms of the
normal, as in Module III and in the thesis. The same distinction between
the interface line and its normal applies to habit planes in 3-D, a
planned extension of this laboratory. The line and the normal pair up as
follows (angles from [10]; a direction and its opposite are the same
line):
line θ
normal (direction)
acute normal angle α
\(\theta_1=\tan^{-1}(1/\sqrt{-t})\)
\(\theta_1+90^\circ\equiv-\alpha\)
\(\tan^{-1}\sqrt{-t}\)
\(\theta_2=180^\circ-\theta_1\)
\(\theta_2-90^\circ=+\alpha\)
\(\tan^{-1}\sqrt{-t}\)
For t = −0.5: lines at 54.74° and 125.26°; normals at 144.74° and
35.26°. With Module III set to “Isotropic elasticity” and \(t=-0.5\), it
lists its zero minima of \(B(\mathbf n)\) at these two normal directions
(sampled at 1°, so near 145° and 35°).
Step 6. Mohr’s circle.
Apply \(\cos^2\theta=\tfrac12(1+\cos2\theta)\),
\(\sin^2\theta=\tfrac12(1-\cos2\theta)\) and
\(2\sin\theta\cos\theta=\sin2\theta\) to the Step 1 entries:
As θ grows, \((\epsilon^0_{nn},\epsilon^0_{nq})\) moves round a circle
with center \(\bar c\) and radius R, turning by −2θ. The vertical axis
is tensor shear; engineering shear is twice it. The circle meets
\(\epsilon^0_{nn}=0\) only if \(R\ge\bar c\), i.e. \(t\le0\), at
the green dots: the same shear \(\epsilon^0_{sm}\) as in Step 4. (The
plot labels the center c; it is \(\bar c\) here to avoid clashing with
\(\cos\theta\).)
Step 7. One case solved completely.
Take \(t=-0.5\), \(\epsilon_\eta=0.01\), and the isotropic stiffness
\(C_{11}=3\), \(C_{12}=1\), \(C_{44}=1\) (dimensionless), which is
Module III’s “Isotropic elasticity” preset. We find the habit line, then compute the
plate energy twice: at the habit normal and at a poor orientation.
Entry by entry:
\(\epsilon^0_{ss}=0.01\cdot\tfrac13-0.005\cdot\tfrac23=0\);
\(\epsilon^0_{mm}=0.01\cdot\tfrac23-0.005\cdot\tfrac13=0.005\);
\(\epsilon^0_{sm}=-0.015\times0.57735\times0.81650=-0.0070711\). Trace
0.005 and determinant \(-5\times10^{-5}\) agree with the original
diagonal matrix. The Mohr readout shows the last entry as
\(-0.7071\,\epsilon_\eta\).
(iv) The frame vectors and the compatible vector a.
\[\mathbf s=\begin{pmatrix}0.57735\\0.81650\end{pmatrix},\qquad \mathbf
m=\begin{pmatrix}-0.81650\\0.57735\end{pmatrix},\qquad \mathbf
a=2\epsilon^0_{sm}\mathbf s+\epsilon^0_{mm}\mathbf m
=\begin{pmatrix}-0.012247\\-0.0086603\end{pmatrix}.\]
Check that it reproduces the eigenstrain in crystal axes:
The skew part is a rotation by 0.0070711 rad (0.41°). The eigenstrain is
exactly a compatible plate deformation plus this rigid rotation.
(v) Stiffness in matrix form. For the in-plane cubic
law with tensor shear,
\(\sigma_{xx}=C_{11}\epsilon_{xx}+C_{12}\epsilon_{yy}\),
\(\sigma_{yy}=C_{12}\epsilon_{xx}+C_{11}\epsilon_{yy}\),
\(\sigma_{xy}=2C_{44}\epsilon_{xy}\). The eigenstress is
Read this physically. \(\sigma_{xx}=0\): the faces (normal x) carry no
traction, as Step 2 demands. \(e_{yy}=0.005\): along the plate the
particle wanted to shrink by 0.005 but the matrix holds its length, so
it is stretched elastically and carries tension 0.0133. The energy
density is \(\tfrac12
e:\sigma=\tfrac12(0.005)(0.013333)=3.33\times10^{-5} =\tfrac12B\).
With Module III set to “Isotropic elasticity” and \(t=-0.5\), its curve
gives \(B=6.67\times10^{-5}\) at normal 0° and
\(2.67\times10^{-4}\) at 90°, and zero at the habit normals.
References. J. D. Eshelby, Proc. R. Soc. Lond. A 241,
376–396 (1957). T. Mura, Micromechanics of Defects in Solids,
2nd ed., Kluwer (1987). A. G. Khachaturyan,
Theory of Structural Transformations in Solids, Wiley (1983).
Try it yourself
Press “t = −1”. Check that the lines are at 45° and 135°, and that the
Mohr circle is centered on the origin.
Drag the t slider slowly from −1 toward 0. Watch θ follow the line and
turn toward [01], and the green dots move together.
Push t above 0. The circle leaves the vertical axis and the habit line
disappears.
Type your own θ (for example 30°). The angle is now free. Move it and
watch P travel round the circle at twice the rate of the plate.
Set t = −0.5, then open Module III, choose “Isotropic elasticity”,
set its t to −0.5, and compare its minimum normal with α = 35.26°
from Step 5.
Computation
The page evaluates \(\epsilon^0_{nn}(\theta)\) directly and solves its
zero condition analytically; no remembered angle is inserted. Positive t
returns no roots and t = 0 is handled as the limit θ = 90°. When θ
follows t, the calculation uses the exact root, and the input box shows
it rounded to four decimals. The plate sketch rotates a prescribed
shape; it is not a kinetic simulation.
Convention note: my thesis Eq. (3.2), p. 20, uses diag(1, t). Eq.
(4.10), p. 48, gives \(\tan^{-1}\sqrt{-t}\) as a line angle from x.
Direct projection under Eq. (3.2) gives that value for the interface
normal, and its complement for the line. This laboratory labels
the line and the normal separately.
KEY RESULT
A stress-free habit line exists only when the principal misfit strains have opposite signs. A thin plate lying along the direction where the misfit extension vanishes fits the matrix without long-range stress.
MODULE II
Eshelby’s inclusion: what jumps at the interface.
What stress does a misfitting inclusion feel, inside and out?
Put the eigenstrain of Module we into an elliptical inclusion inside a
homogeneous matrix. Eshelby’s solution gives the uniform strain inside.
Pick any point on the interface to see which strain and stress components
are continuous there, which jump, and by how much. Then flatten the
ellipse into a thin plate and rotate it.
Jump conditions at the chosen point, (s, m) frame.
Green rows are continuous; orange rows jump.
See the whole field.
The map uses the selectable periodic FFT grid. The profiles below instead
evaluate the uniform interior and the spatially varying exterior of an
isolated ellipse in an infinite matrix separately. Both branches end at
their analytical one-sided interface values. Dashed vertical connectors
mark actual jumps; no interpolation or smoothing crosses the interface.
Periodic map values can differ from these infinite-matrix profiles.
Why did this happen?Physics: the inclusion, its interface and its limits
Eshelby’s uniform interior
Module we described Eshelby’s cut, force back, weld and release
experiment. Its remarkable result is that for an ellipse (an ellipsoid
in 3-D) in a homogeneous infinite matrix, the constrained strain inside
is uniform, whatever the aspect ratio and orientation. The
inclusion also turns rigidly by a small angle ω. The panel on the left
shows three outlines: the hole, the shape the inclusion would take if it
were free, and the shape it actually takes.
The interface is local
At every point of the interface the two jump conditions of Module we
hold, with the local normal \(\mathbf m\) and tangent \(\mathbf s\):
welding keeps the displacement continuous, so \(\epsilon_{ss}\) is
continuous; force balance keeps the traction \(\sigma\mathbf m\)
continuous, so \(\sigma_{sm}\) and \(\sigma_{mm}\) are continuous. The
other components, \(\epsilon_{sm}\), \(\epsilon_{mm}\) and
\(\sigma_{ss}\), jump. The size of the jump depends only on \(\mathbf
m\), the eigenstrain and the stiffness. It does not depend on the
inclusion’s shape. The shape only sets the uniform field inside; the
field just outside is that interior field minus the jump.
From circle to thin plate
For a circle the matrix pushes back from every direction, and the
interior keeps a mix of all components. As the ellipse flattens, its
long faces dominate. The matrix beside those faces becomes unstrained,
so the interior field becomes exactly the jump across the faces: the
thin plate of Module I. Its energy per unit area approaches
\(\tfrac12B(\mathbf m)\). If the plate lies along a habit line, that
limit is zero; otherwise a remnant stress \(\sigma_{ss}\) stays trapped
along the plate.
Orientation
Rotating the ellipse changes which direction carries the long interface.
For a thin plate the energy follows \(\tfrac12B(\mathbf m)\) and is
lowest at the habit orientation. A rounder inclusion averages over many
normals, so its energy depends less on orientation.
Mathematics: interior field, jumps and limits
Step 1. The interior displacement gradient.
Let the ellipse have semi-axes a (along the angle φ) and b. For a
direction n write \(Q(\mathbf n)_{ik}=C_{ijkl}n_jn_l\),
\(\sigma^0=C:\epsilon^0\) and
\[\mathbf g(\mathbf n)=Q(\mathbf n)^{-1}\,\sigma^0\mathbf n .\]
The Fourier solution of equilibrium gives the total strain of any
inclusion as \(\tilde\epsilon(\mathbf k)=\operatorname{sym}\big(\mathbf
g(\hat{\mathbf k})\otimes\hat{\mathbf k}\big)\,\tilde\theta(\mathbf k)\),
where \(\theta\) is 1 inside and 0 outside. For an ellipse the transform
of θ depends on \(\mathbf k\) only through one elliptic radius, and the
inverse transform at any interior point reduces to an average over
directions (Mura, §11):
w is Eshelby’s elastic energy per unit inclusion area (matrix energy
included). The integral reproduces Mura’s closed-form isotropic Eshelby
tensor to machine precision, and it works unchanged for the anisotropic
cubic law.
Step 2. The jump at a boundary point.
At a point with outward normal \(\mathbf m\), Hadamard’s condition gives
\([\![\epsilon]\!]=\operatorname{sym}(\mathbf g\otimes\mathbf m)\) for
some \(\mathbf g\), and traction continuity \([\![\sigma]\!]\mathbf
m=\mathbf 0\) with \([\![\sigma]\!]=C:([\![\epsilon]\!]-\epsilon^0)\)
gives \(Q(\mathbf m)\mathbf g=\sigma^0\mathbf m\). So
The jump is the thin-plate field of Module I for the normal \(\mathbf
m\): it is fixed locally, independent of shape. The table rotates each
tensor into the \((\mathbf s,\mathbf m)\) frame with the sandwich rule
of Module I, Step 1.
Step 3. The two limits.
Thin plate (\(b/a\to0\)): \(\mathbf n\) points along
\(\pm\mathbf m_0\), the normal of the long faces, for almost every
\(\vartheta\). Then \(D\to\mathbf g(\mathbf m_0)\otimes\mathbf m_0\),
the field outside the faces vanishes, and \(w\to\tfrac12B(\mathbf
m_0)\). Circle (\(b=a\)): \(\mathbf n\) is spread
evenly; for isotropic stiffness and a dilatation
\(\epsilon^0=\epsilon\,I\) (plane strain) the interior strain is
\(\epsilon^c=\epsilon\,I/[2(1-\nu)]\).
Step 4. The field maps.
The maps solve the same equation on a periodic cell (1024 × 1024 by
default; 256 and 512 are offered for quicker comparison):
\(\tilde\epsilon(\mathbf k)=\operatorname{sym}(\mathbf g(\hat{\mathbf
k})\otimes\hat{\mathbf k})\tilde\theta(\mathbf k)\) for \(\mathbf k\ne0\),
mean total strain zero, and \(\sigma=C:(\epsilon-\theta\epsilon^0)\).
The profiles along \(\mathbf m\) through the chosen point are the exact
analytic interior and exterior solutions of Step 2, not samples of the
periodic numerical field.
Try it yourself
Press “Circle”, set t = 1 (pure dilatation) and click round the
boundary. The jump table changes with m, but the interior summary does
not: the interior is uniform.
Set t = −0.5, press “Thin plate” and “Align with habit line”. The
energy drops to nearly zero and \(\sigma_{ss}\) on the long face
vanishes. Now press “Worst orientation”.
Drag the aspect-ratio slider from 1 to 0.01 and watch w approach the
dashed thin-plate limit.
Choose the map component \(\sigma_{xy}\) and move the interface point.
In the profiles, the continuous components meet at the same one-sided
interface value while the discontinuous components have distinct
one-sided limits.
Press “AZ = 3 stiffness”. The jump rule is unchanged, but
the energy-orientation curve changes shape.
Computation
The interior field is the angular integral of Step 1 with 4096 midpoint
samples (2048 for the sweeps), which resolves aspect ratios down to
0.01. Jumps use Step 2 exactly. The energy sweeps recompute Step 1 for
41 aspect ratios and 91 orientations.
The field maps use a 1024 × 1024 FFT grid by default (256 and 512 are
selectable) on a periodic unit cell with an inclusion of semi-axis a =
0.16, a 4 × 4 supersampled indicator, and zero mean total strain.
Periodic images and the finite area fraction shift the interior values
by a few per cent relative to the infinite-matrix solution, and the
sharp interface shows small Gibbs ripples. The separate sharp-interface
profiles use the actual selected aspect ratio and a singularity-removing
angular substitution, with 2048 midpoint samples per exterior point. The
maps use b/a ≥ 0.08, the thinnest plate the grid resolves.
KEY RESULT
Inside an elliptical inclusion the strain is uniform. At the interface, only the components not fixed by welding and force balance jump, and the size of the jump depends on the interface normal, not on the inclusion’s shape.
MODULE III
Elastic energy and directional dependence.
How does elastic anisotropy choose the cheapest direction?
Change this module’s eigenstrain and elastic constants independently. The
plots calculate the self elastic energy kernel \(B_{pp}(\mathbf n)\),
using the same eigenstrain on both sides of the contraction. They do not
plot a cross kernel or Young’s modulus. The polar angle denotes the
Fourier wavevector direction: a
modulation normal, not a plate tangent.
Ni superalloy γ′ uses the room-temperature stiffness of nickel, \(C_{11}=246.5\), \(C_{12}=147.3\), \(C_{44}=124.7\) GPa, entered in units of 100 GPa, and a dilatational γ/γ′ misfit of magnitude 0.3%. The sign of the misfit varies between alloys; \(B(\mathbf n)\) depends only on its square.
The eigenstrain is
\(\boldsymbol\epsilon^{(p)}=\epsilon_p\operatorname{diag}(1,t)\). These
inputs belong only to Module III. Equal components, \(t=1\), give in-plane
dilatation. Unequal components can give a different angular symmetry, even
with isotropic elastic constants. The self kernel has energy-density units
for dimensional stiffnesses; this widget uses scaled model values.
Read this polar plot as an energy plot
The radius is proportional to \(B_{pp}(\mathbf n)\), with zero at the
center.
The concentric circles label kernel values. The drawing is scaled to fit
the panel, so compare the labeled values when changing parameters. A
minimum lies closer to the center. Module IV uses a labeled signed scale
instead, because a cross kernel can be negative.
A surface-energy plot uses radius \(\gamma(\mathbf n)\), where \(\gamma\)
is interfacial energy per area. This plot uses the elastic kernel, which
depends on stiffness, eigenstrain and mechanical relaxation. Both are
functions of direction, but they need not have the same angular shape.
Neither raw polar curve is automatically the equilibrium particle shape: a
surface-energy shape requires a Wulff construction, while an elastic
particle shape requires the total elastic and interfacial energies.
Try the limiting case. Select equal dilatational
components and isotropic elasticity. The kernel is independent of
direction and the polar curve is a circle. Keeping isotropic stiffness but
changing the strain ratio can restore angular variation. With cubic
anisotropy and equal components, the curve has the corresponding fourfold
symmetry. Ideal plate tangents are perpendicular to the plotted modulation
normals.
Why did this happen?Physics
Eigenstrain specifies what the phase wants to do. Stiffness specifies
the cost of preventing it. Mechanical relaxation reduces that cost.
Their combination gives B(n). A minimum identifies a low-penalty
modulation normal; the corresponding ideal plate is perpendicular to it.
Several equal minima are symmetry-related choices.
Mathematics
From my Appendix A, Eqs. (A.1–A.12), pp. 107–111. This
is the elastic-energy derivation developed using Khachaturyan’s
microelasticity framework. Spatial indices \(i,j,k,l\) are summed; phase
indices \(p,q\) are summed only where shown. The laboratory uses two
spatial dimensions.
Step 1: Separate eigenstrain, mean strain and periodic relaxation.
For homogeneous stiffness and zero applied mean stress,
\(E_{ij}=\langle\epsilon^0_{ij}\rangle\). The mean terms cancel in the
six-integral expansion of Appendix A. Only the fluctuations
\(\Delta\theta_p=\theta_p-\langle\theta_p\rangle\) remain.
Step 2: Solve equilibrium for each nonzero Fourier mode.
\(B_{pq}\) is the elastic energy kernel. Its first term
is the unrelaxed eigenstrain contraction; the second is the energy
reduction from mechanical relaxation. It becomes a total energy only
after weighting by the field spectra and summing or integrating over
modes. This is Eq. (A.12), with \(d=2\) here.
Step 4: Differentiate the energy: Appendix B, Eqs. (B.1–B.12).
Here \(a\) is a fixed field label, not a summed spatial index. The two
equal variations of the quadratic form cancel its factor of one half. We
use \(B_{aq}=B_{qa}\), renaming dummy indices explicitly. For
\(\theta_a=\eta_a^2\), the chain rule gives \(\delta
F_e/\delta\eta_a=2\eta_a g_a\) in real space.
Boundary-condition distinction: Appendix A uses a
relaxed mean strain. The finite-plate module fixes \(E_{ij}=0\) and
therefore retains the additional mean energy
\(\tfrac{V}{2}(E-\langle\epsilon^0\rangle):C:(E-\langle\epsilon^0\rangle)\).
Its zero mode must not be silently dropped.
\(A_Z=2C_{44}/(C_{11}-C_{12})\). The 2-D law uses the in-plane cubic
sub-block, with tensor shear \(\sigma_{xy}=2C_{44}e_{xy}\), no
out-of-plane eigenstrain, and no plane-stress condensation.
For every sampled direction, form the 2 × 2 acoustic tensor Q, invert it
and contract the stress vectors. Stability checks reject invalid
constants. All minima come from evaluated curves. Flat curves are
reported as directionally degenerate. This module’s self-kernel plot
uses a direct radial scale with zero at the center; the signed cross
kernels of Module IV use a labeled offset scale, so negative values are
never folded onto positive radii.
KEY RESULT
The elastic energy of a composition modulation depends on its direction. The minimum of \(B(\mathbf n)\) marks the modulation normal that allows the most relaxation, so elastic anisotropy alone can give a dilatational misfit a preferred direction.
MODULE IV
Sandeep’s thesis example: two precipitate phases in one matrix
How do two precipitate phases interact elastically?
This module introduces the three-phase system studied in Sandeep
Sugathan’s thesis. The matrix is \(\alpha\); the two precipitate phases
are \(\beta\) and \(\gamma\). Both precipitates have a dilatational misfit
relative to \(\alpha\): their stress-free size differs from that of the
matrix, without a preferred strain direction. In the X2
example, \(\beta\) expands by 1% and \(\gamma\) contracts by 1%.
The elastic moduli are homogeneous and anisotropic.
Homogeneous means that the same stiffness tensor \(C_{ijkl}\) is used in
all three phases. Anisotropic means that the elastic response depends on
direction. These are different properties: equal moduli across phases do
not mean isotropic moduli.
The thesis reference is Chapter 5, Tables 5.1–5.2, Eq. (5.1) and Fig.
5.18. The parameters are \(G=2000\), \(\nu=1/3\), \(A_Z=3\),
\(\epsilon_\beta=0.01\) and \(\epsilon_\gamma=-0.01\). Here \(G\) is the
modulus parameter used in the thesis, \(\nu\) is Poisson’s ratio, \(A_Z\)
is the Zener anisotropy ratio, and \(\epsilon_p\) is the stress-free
linear misfit of precipitate phase \(p\) relative to \(\alpha\). Strains,
\(\nu\) and \(A_Z\) are dimensionless. The stiffness and energy values
below use the thesis’s model units; they are not labeled as pascals or
joules without a dimensional conversion.
Set the elastic constants
Change each stiffness independently here. Alternatively, change the shear
parameter \(\mu\) and Zener anisotropy ratio \(A_Z\), using a fixed
Poisson parameter \(\nu=1/3\). The shear-parameter conversion uses a fixed
\(\nu=1/3\). Direct stiffness inputs remain independent; an arbitrary
triple need not correspond to that fixed Poisson parameter. These
constants belong only to Module IV.
The stiffness constants and \(\mu\) use the same energy-density scale.
This demonstration uses scaled values; no conversion to pascals is
assumed. For an anisotropic solid, \(\mu\) and \(\nu\) are the parameters
in the conversion below, rather than a shear modulus and Poisson ratio for
every direction. When \(A_Z=1\), they reduce to the usual isotropic
values.
Use \(\mu>0\), \(A_Z>0\), \(\nu<1/2\) and \(1+3A_Z+4\nu>0\)
(for \(A_Z=1\) this reduces to the isotropic range \(-1<\nu<1/2\)). Independent
stiffness inputs must satisfy \(C_{44}>0\), \(C_{11}-C_{12}>0\), and
\(C_{11}+2C_{12}>0\). Invalid inputs produce an explanation and retain
the last valid plots.
At \(A_Z=3\), a dilatational self kernel favors Fourier directions
\(\langle10\rangle\). Opposite misfits reverse the sign of the cross
kernel, whose minimum is then along \(\langle11\rangle\). The pair-energy
graph separately calculates the preferred separation direction by summing
all Fourier modes.
Explore the three kernels
Select Sandeep thesis example to load the anisotropic
reference case. Select Isotropic comparison to retain the
misfits and set \(A_Z=1\). The stiffness controls above affect only Module
IV. Misfits and strain ratios update the plots as you type. Keeping both
ratios at one gives dilatational misfit; changing a ratio introduces
non-dilatational strain and leaves the thesis example’s assumptions.
Read the signed values. Each polar panel displays one
kernel: \(B_{\beta\beta}\), \(B_{\gamma\gamma}\), or \(B_{\beta\gamma}\).
All three use the same scale. The bold circle marks zero; values inside it
are negative and values outside it are positive. Moving inward means a
lower signed value. Green dots mark the minimum. The angle is the Fourier
normal direction \(\mathbf n\), measured from [10].
For equal and opposite misfits, the two self kernels are identical and the
cross kernel is their negative. Separate panels let you see all three
without hiding coincident curves. These are kernel plots; they do not show
particle shapes.
Why did this happen?
When is the β–γ cross coefficient important?
The cross coefficient measures elastic coupling between the two phase
fields. It is not the interaction energy of two particles. For the
homogeneous elastic constants and dilatational misfits used here, all
three kernels contain the same directional function:
Here \(\epsilon_\beta\) and \(\epsilon_\gamma\) are dimensionless linear
misfits relative to the matrix. The unit vector \(\mathbf n\) gives the
Fourier wavevector direction. The function \(K\) is the elastic kernel for
unit dilatational misfit; it depends on the elastic constants and
direction. The kernels have the dimensions of energy per volume when
dimensional stiffnesses are used. This widget displays them in the model
energy-density units defined above.
Thus the cross coefficient is comparable to both self coefficients when
the misfit magnitudes are comparable. For Sandeep’s equal-and-opposite
example, \(\epsilon_\beta=0.01\) and \(\epsilon_\gamma=-0.01\), so
\(B_{\beta\gamma}=-B_{\beta\beta}=-B_{\gamma\gamma}\) at every direction.
There is no anisotropy threshold at which the cross coefficient suddenly
appears.
A large cross coefficient does not by itself establish a large particle
interaction.
The interaction energy also depends on the amounts, shapes, separation and
arrangement of both phase fields. Contributions from different Fourier
modes can reinforce or cancel. Elastic anisotropy gives the kernel angular
variation; a nonzero isotropic cross coefficient alone does not establish
an arrangement-dependent interaction. The Bitter–Crum derivation below
explains the isotropic limit.
Now calculate a particle-pair energy.
The thesis preset selects a β–γ pair with opposite misfits. For this case
at \(A_Z=3\), [11] has lower interaction energy. A β–β or γ–γ pair has
same-sign misfits and gives a different preference. The positive self
kernels are higher along [11]; the signed β–γ cross kernel is lower there.
The three polar panels use signed radial values; a smaller radius means a
lower kernel value.
Why did this happen?Physics
Changing one misfit sign reverses the cross coupling because it is
bilinear in the two eigenstrains. Both self terms remain nonnegative.
However, \(B_{\beta\gamma}(\mathbf n)\) is a reciprocal-space
coefficient. To obtain real-space interaction energy at separation R, we
must also include particle shape spectra and Fourier phases.
Single-particle energy and pair-interaction energy are different
quantities.
The \(\mathbf k=0\) coefficient in this clamped periodic calculation is
\(\epsilon^\beta:C:\epsilon^\gamma\). The square contains identical
circular Gaussian profiles h, with width 0.045 of the box. Each Fourier
mode contributes; the kernel is not simply evaluated at the separation
angle.
Computation
Use a 64 × 64 periodic square and exact Fourier translations of the
sampled Gaussian. Evaluate a 1° separation-angle sweep. Periodic copies
are included. The profiles have diffuse tails. The on-screen circles
indicate their positions, not sharp boundaries.
Thesis reference: Sandeep Sugathan, Chapter 5, Tables
5.1–5.2 (p. 116), Eq. (5.1) and Fig. 5.18 (p. 133), discussion p. 132.
The X2 example has G = 2000, ν = 1/3, AZ = 3 and
misfits ±0.01. Eqs. (3.27–3.29) give \(C_{11}=7000\), \(C_{12}=5000\),
\(C_{44}=3000\). Press “Sandeep thesis example” to see the comparison
table: the self terms are 0.342857 along ⟨10⟩ and 0.8 along ⟨11⟩, and
the cross term is their negative. The separate two-Gaussian experiment
is a teaching calculation, not a reproduction of the thesis’s full
phase-field microstructure.
When does the interaction control the arrangement?
For the two prescribed circular profiles in this widget, rotating their
separation leaves each self energy unchanged. The angle-dependent
interaction therefore selects the preferred separation direction. In the
thesis example, opposite misfits with \(A_Z=3\) give the lowest pair
interaction along [11]. The self kernels still favor Fourier normals
along [10].
Use the pair calculation to compare actual arrangements, rather than
reading a pair direction directly from the kernel polar plot. Define
Here \(E_{\mathrm{int}}\) is the interaction energy reported by this
widget in its normalized model units. The directions [10] and [11]
describe the line joining the particle centers; they are different from
the Fourier normal \(\mathbf n\) in the kernel plots. A negative
difference favors [11], a positive difference favors [10], and zero
gives no preference between these two arrangements. This comparison keeps
particle size, separation and elastic constants fixed. It does not exclude
a lower energy at another angle.
In an evolving microstructure, the precipitates can also change shape and
composition. The change in interaction energy must then be compared with
changes in self elastic energy, interfacial energy and chemical free
energy. Larger misfits increase elastic effects relative to the nonelastic
contributions when other parameters are fixed. Both precipitate phases
must have appreciable misfits and spatially coupled fields for their cross
contribution to be important. Increasing anisotropy can strengthen a
directional preference, but it does not give a universal threshold for
interaction dominance.
For one Fourier mode, define \(S_\beta=B_{\beta\beta}|\tilde h_\beta|^2\),
\(S_\gamma=B_{\gamma\gamma}|\tilde h_\gamma|^2\), and
\(X=2B_{\beta\gamma}\operatorname{Re}(\tilde h_\beta\tilde h_\gamma^*)\). The
mode energy is \((S_\beta+S_\gamma+X)/2\). The cross contribution is most
significant when both self contributions are comparable and the Fourier
phases give strong correlation. Mechanical stability gives \(|X|\leq
S_\beta+S_\gamma\): the interaction can control the preferred arrangement
without exceeding the sum of the self contributions in magnitude. The full
phase-field calculation is needed to decide the final morphology.
Derivation and the Bitter–Crum limit
Step 1: The transformation strain of each phase
Let \(h_\beta(\mathbf x)\) and \(h_\gamma(\mathbf x)\) be dimensionless
fields describing where the precipitates are located. A field is one
inside its phase and zero outside for a sharp interface; a smooth field
can represent a diffuse interface. The position is \(\mathbf x\). Taking
the matrix as the zero-misfit reference gives
Here \(\epsilon^0_{ij}\) is the prescribed transformation strain, and
\(\delta_{ij}\) is one when \(i=j\) and zero otherwise. The indices
identify Cartesian components. A three-dimensional dilatation has three
equal diagonal components.
This widget uses the two-dimensional in-plane elastic law described
in Module III:
\(\boldsymbol\epsilon^p=\epsilon_p\operatorname{diag}(1,1)\). It omits
the out-of-plane transformation strain; it is not a full
three-dimensional plane-strain reduction.
Step 2: Impose mechanical equilibrium
The displacement components are \(u_i\). The total strain is
\(\epsilon_{ij}=(\partial_i u_j+\partial_j u_i)/2\), where
\(\partial_i\) denotes differentiation with respect to position
component \(x_i\). Elastic strain is total strain minus transformation
strain. Stress \(\sigma_{ij}\) and elastic energy \(E_{\mathrm{el}}\)
are therefore
Repeated indices are summed. \(V\) is the body volume; the
two-dimensional calculation uses area and energy per unit out-of-plane
thickness. Stiffness and stress have units of pressure in a dimensional
model, and the integral then has units of energy. Mechanical equilibrium
assumes no body force. The displacement adjusts to reduce the energy
while satisfying the boundary conditions.
Step 3: Solve each nonzero Fourier mode
A Fourier mode has wavevector \(\mathbf k\), with units of inverse
length in a dimensional model. Its unit normal is \(\mathbf n=\mathbf
k/|\mathbf k|\). Define the stress associated with the prescribed
strain, the acoustic tensor, and the inverse acoustic tensor by
\(Q\) describes the directional stiffness of the mode. \(\Omega\) has
units of inverse stiffness. With the Fourier convention
\(\widetilde{\partial_j u_i}=\mathrm i k_j\tilde u_i\), mechanical
equilibrium gives
Here \(\mathrm i^2=-1\), a hat denotes a Fourier coefficient, and
\(\tilde\sigma^0_{ij}=\sum_p\sigma^p_{ij}\tilde h_p\). Substituting this
equilibrium displacement into the energy removes the displacement as an
independent unknown.
Step 4: Obtain the two self kernels and one cross kernel
The first term is the energy coefficient before displacement relaxation.
The second term is the reduction produced by mechanical relaxation. The
vector \(a^p_i\) is the traction associated with the prescribed strain
on a plane normal to \(\mathbf n\). Each \(B_{pq}\) has units of energy
density in a dimensional model.
For clarity, define \(\tilde h_p(\mathbf k)=V^{-1}\int_V h_p(\mathbf
x)e^{-\mathrm i\mathbf k\cdot\mathbf x}\,dV\) in a periodic body. These
coefficients are dimensionless. The nonzero-mode energy density is
\(\operatorname{Re}\) means real part, and an asterisk means complex
conjugate. The two self kernels describe each precipitate phase’s
contribution. The cross kernel describes the coupling between their
fields. Symmetry gives \(B_{\beta\gamma}=B_{\gamma\beta}\), so there are
three independent kernels, although the system contains three phases.
The matrix contributes through the common stiffness and the reference
strain.
For the two-dimensional square-symmetric stiffness, write
\(n_x=\cos\theta\) and \(n_y=\sin\theta\), where \(\theta\) is the
wavevector-normal angle. The matrix actually inverted by the widget is
The thesis parameters give \(C_{11}=7000\), \(C_{12}=5000\),
\(C_{44}=3000\) in model units. The equal and opposite misfits imply
\(B_{\beta\beta}=B_{\gamma\gamma}\) and
\(B_{\beta\gamma}=-B_{\beta\beta}\). For this in-plane calculation, the
self coefficient is \(0.342857\) along [10] and \(0.8\) along [11]; the
cross coefficient is their negative. These numbers check the kernel
calculation, not the reproduction of a complete thesis microstructure.
Step 5: Derive the Bitter–Crum theorem from the isotropic kernel
The isotropic example demonstrates the Bitter–Crum theorem.
We can show why it holds by calculating \(B_{pq}\). Assume that the
elastic moduli are the same in all phases, the elasticity is isotropic,
and each phase has a purely dilatational transformation strain. Here the
phase fractions and misfits are fixed. The calculation uses an infinite body or the
compatible periodic boundary conditions described below.
For the two-dimensional in-plane law used here, let \(\lambda=C_{12}\)
and \(\mu=C_{44}\) be the Lamé elastic constants. Both have units of
pressure in a dimensional model. Isotropy requires
\(C_{11}=\lambda+2\mu\), or \(A_Z=1\). Since
\(\epsilon^p_{ij}=\epsilon_p\delta_{ij}\), the prescribed stress is
\(\sigma^p_{ij}=2(\lambda+\mu)\epsilon_p\delta_{ij}\). Thus
Here \(I\) is the identity matrix, and \(\mathbf n\otimes\mathbf n\) has
components \(n_i n_j\). Substitute these expressions into the kernel.
The two terms give
The coefficient \(K_B\) has units of pressure.
There is no direction \(\mathbf n\) left in this expression.
Equal and opposite misfits give \(B_{\beta\gamma}=-B_{\beta\beta}\), but
this negative coefficient alone does not imply attraction between
precipitates. We must substitute it into the complete energy expression.
Define the scalar misfit field \(e(\mathbf x)=\epsilon_\beta
h_\beta(\mathbf x)+\epsilon_\gamma h_\gamma(\mathbf x)\). It is
dimensionless. Parseval’s identity states that the sum of the squared
Fourier coefficients equals the spatial average of the squared field.
Removing the zero mode therefore gives
Angle brackets denote the spatial average. For disjoint phase regions,
\(h_p\) is one inside phase \(p\) and zero outside. Consequently
\(h_p^2=h_p\) and \(h_\beta h_\gamma=0\). If \(f_p=\langle h_p\rangle\)
is the dimensionless phase fraction, then
This is the Bitter–Crum result in this model. The
energy depends on the phase fractions and misfits. It does not depend on
precipitate shape, position, separation or arrangement. Moving disjoint
precipitates while keeping their amounts fixed does not change the
energy: there is no elastic interaction driving their relative motion.
Opposite misfits do not change this conclusion.
For imposed mean strain \(\bar\epsilon\), add
\(E_0/V=\tfrac12(\bar\epsilon-\langle\epsilon^0\rangle):C:(\bar\epsilon-\langle\epsilon^0\rangle)\).
The colons denote tensor contraction. This term also depends only on the
mean transformation strain when the imposed strain is fixed. At relaxed
zero mean stress, it vanishes. Comparing arrangements at fixed phase
amounts is essential; a cross term obtained by subtracting two separate
clamped calculations is not, by itself, a separation-dependent
interaction.
Select Isotropic comparison to check the constant
kernel numerically. Its circle and the horizontal signed curves
demonstrate the directional cancellation derived above; the energy
reduction proves the shape-and-arrangement independence. With
anisotropic moduli, the kernel generally retains its directional
dependence, and this Bitter–Crum proof no longer applies. Eshelby’s
uniform-interior-strain theorem for an ellipsoidal inclusion is a
separate result.
KEY RESULT
Besides each phase’s own elastic energy, two phases interact through a cross term that is bilinear in their misfits. With opposite misfits the cross term can be negative, so the elastic interaction can favour particular relative positions of the two phases.
MODULE V
Soft or hard: rotate a fixed plate.
Does a soft or a hard plate prefer a different orientation?
For this prescribed thin plate, what orientation minimises the elastic
energy? The crystal axes and eigenstrain stay fixed while the plate shape
rotates. Choose β or γ; each retains its own stiffness and eigenstrain
settings. This module contains one plate at a time.
The selected phase uses the misfit inputs in this module. Its matrix and
precipitate constants are also independent of every other module.
Choose parameters and calculate a sweep.
Why did this happen?Physics
Soft and hard refer to the elastic response relative to the matrix. The
same eigenstrain is accommodated differently when stiffness varies in
space. With isotropic phases and dilatational misfit, an infinite medium
has no preferred material direction. Small angular differences in this
periodic calculation require particular care: the square cell and finite
grid also introduce directions. We fix the plate shape to isolate its
orientation energy, rather than claim to predict its unconstrained
equilibrium morphology.
Physical insight: A minimum is the smallest elastic
penalty among the sampled orientations of this prescribed plate, under
the stated boundary condition. It is not automatically a habit plane or
a stress-free state.
Mathematics
Inhomogeneous equilibrium: Bhattacharyya, Heo, Chang
and Chen, Communications in Computational Physics 11 (2012),
726–738, Eqs. (2.6–2.16). Tushar Jogi’s thesis, §§3.1.4–3.1.6 and
Appendix B, supplies the related phase-field formulation and
driving-force derivation. Indices are retained here so each contraction
can be checked.
The wave-number factor follows directly by transforming two spatial
derivatives. If the Green tensor is defined using \(k_jk_l\), its
inverse already contains \(|\mathbf k|^{-2}\). If it is defined using
the unit direction \(n_jn_l\), that factor must appear explicitly. The
zero mode is handled separately.
For prescribed mean stress, invert \(\langle C\rangle\) on symmetric
tensors. In general \(\langle C\rangle^{-1}\ne\langle C^{-1}\rangle\).
This is the meaning of the compliance-like quantity defined in CICP Eq.
(2.16). The current plate experiment instead prescribes \(E=0\); it does
not claim to solve a traction-free macroscopic cell.
Elastic driving force, with the interpolation distinguished from the
kernel.
This is the first-order result of Tushar’s Appendix B, pp. 181–182,
written in indicial form. The displacement variation vanishes at
mechanical equilibrium under the chosen boundary conditions. For this
laboratory, \(C=C^m+h(C^p-C^m)\) and \(\epsilon^0=h\epsilon^p\), so
\(g_h=\tfrac12 e:(C^p-C^m):e-\sigma:\epsilon^p\). The scalar
interpolation called \(B(\phi)\) in Tushar’s thesis is not the
elastic energy kernel \(B_{pq}(\mathbf n)\).
The production solver uses preconditioned conjugate gradients rather
than the paper’s fixed-point iteration. Both solve the same
heterogeneous equilibrium equation. An independent CICP-style spectral
iteration is included in the validation suite for comparison. A spectral
symmetric-gradient operator and its adjoint form A = D* C(x) D.
Preconditioned conjugate gradients solve A u = D* C(x) ε⁰. A homogeneous
acoustic inverse is only a preconditioner; the residual uses the full
heterogeneous stiffness. Failed solves are rejected, not plotted as
minima.
The unit square contains a smooth ellipse with semiaxes 0.22 and 0.045.
Its diffuse area is held at π × 0.22 × 0.045 for every orientation. The
tanh transition width is 0.18 in elliptic-radius units. Fourier
derivatives on even grids set Nyquist derivatives to zero, consistently
in both the solver and reference. These modes retain their unrelaxed
energy. Refine the grid to check their influence and resolve the
interface.
Circles on the plots mark sampled local minima; larger circles mark
sampled global minima. Recalculate at 64² or 128² and a smaller angular
step to assess convergence. The solver reports its residual and
iterations. The “Homogeneous limit” copies matrix constants to the
selected plate and compares against an independent Fourier-energy
evaluation.
KEY RESULT
When the plate is softer or stiffer than the matrix, its preferred orientation is set by how much of the misfit the stiffness contrast lets the solid relax, so a finite plate need not lie along the zero-extension line of an infinite plate.
Equations, numerical checks and source code
We compare the calculated strains and elastic energies with known solutions
and with results from separate implementations. We also repeat selected
calculations at finer grid sizes and smaller angle steps to check how much
the results change.
Numerical details
The saved numerical results and explanations of the checks are available below.
This laboratory is part of my teaching and research in mesoscale
microstructure modeling. It connects eigenstrain, elastic equilibrium and
elastic energy with microstructure, complementing our teaching notebooks
and research codes for homogeneous and inhomogeneous elasticity,
phase-field evolution and ferroelectric modeling.
Explore the corrected course notebook Elastic.ipynb, a direct
iterative perturbative solver and an equivalent-eigenstrain solver. Each
notebook derives the equations, exposes the iteration and lets you change
the physical parameters.
We provide these doctoral theses for readers who want the full formulations and results. If you use their formulations, results, figures or code, please acknowledge the thesis author, cite the thesis and cite the relevant published articles. The paper links below provide starting points; each thesis lists further publications.
My historical hexagonal-to-orthorhombic codes
and Julia thesis model
describe elastic effects on microstructural evolution. The historical repository includes the GSL version.
The Julia model includes conserved noise in composition, separate nonconserved noise in all three variants,
and my particle-moment utility for measuring changes in particle shape. Each repository describes its equations and tests.
We discuss phase separation inside a particle
with the Cahn–Hilliard example, including the role of the field that distinguishes the particle from its surroundings.
From my thesis: a growing precipitate tilts.
Saswata Bhattacharyya, Fig. 4.4, p. 47: t = −0.5, G = 750, c∞ = 0.2.
Contours at times 20, 260, 500, 760 and 980 in a 140 × 140 domain.
Interfacial energy and growth affect the finite shape; the
invariant-line construction supplies a limiting compatibility argument.
Sources: Saswata Bhattacharyya,
Evolution of Multivariant Microstructures with Anisotropic Misfit: A
Phase Field Study, Appendix A, Eqs. (A.1–A.12), pp. 107–111; Appendix B, Eqs. (B.1–B.12),
pp. 112–114; and the habit-line discussion in Chapter 4. These derivations
follow A. G. Khachaturyan,
Theory of Structural Transformations in Solids (Wiley, 1983).
Tushar Jogi, Computational Modeling and Simulations of Process-Microstructure-Property Relations in Model Ni-base Superalloys, IIT Hyderabad, September 2021, Chapter 3 and Appendix B, pp. 181-182, supplies the phase-field and elastic driving-force reference used in Module V.
Other reference examples: Sandeep Sugathan,
A Phase-Field Study of Elastic Stress Effects on Phase Separation in
Ternary Alloy Systems, IIT Hyderabad, June 2019, Chapters 3 and 5 as cited in Module IV.
Read the elastic-kernel and driving-force derivations.
Contributions to this laboratory
Tushar Jogi
Tushar carried out his PhD research with me on microstructural evolution and deformation in Ni-base superalloys (IIT Hyderabad, 2021). We developed a phase-field model for coherent precipitates with elastic anisotropy, stiffness contrast and applied stress, and he implemented the iterative perturbation method for elastically inhomogeneous solids. His elastic driving-force derivation is the reference for Module V. He also introduced superellipsoidal inclusions into ParaDiS to study precipitate–dislocation interactions, and plans to release this module for OpenDiS. Tushar is now a Postdoctoral Researcher at the Max Planck Institute for Sustainable Materials, Germany.
Sandeep Sugathan
Sandeep carried out his PhD research with me on elastic stress effects on phase separation in ternary alloys (IIT Hyderabad, 2019). His ternary elastic formulation is implemented directly in Module IV, which calculates the elastic coefficients for two precipitate phases in one matrix; its X2 example is one of the laboratory's reference checks. The conversion between cubic stiffnesses and the Schmidt–Gross parameters follows Chapter 3 of his thesis. Sandeep is now a Research Professor at Kookmin University, South Korea.
Soumya Bandyopadhyay
Soumya carried out his PhD research with me on electromechanical effects on domain evolution and polarization switching in ferroelectric perovskite oxides (IIT Hyderabad, 2020). He contributed the ferroelastic formulation and, in our research, implemented the virtual eigenstrain method of Khachaturyan's microelasticity theory for elastically inhomogeneous solids; the equivalent-eigenstrain solver on my inhomogeneous elasticity page is inspired by that work. Soumya is now a Postdoctoral Research Associate at the University of Florida, USA.